breakdown. Some electrode systems for testing in air make use of pressure gaskets around the electrodes to prevent flashover. The material of the gaskets or seals around the electrodes has the potential to influence the breakdown values. 
6.4.1 When tests are made in insulating oil, an oil bath of adequate size shall be provided. (Warning—The use of glass containers is not recommended for tests at voltages above about 10 kV, because the energy released at breakdown has the potential to be sufficient to shatter the container. Metal baths must be grounded.) 
It is recommended that mineral oil meeting the requirements of Specification D3487, Type I or II, be used. It shall have a dielectric breakdown voltage as determined by Test Method D877 of at least 26 kV. Other dielectric fluids are suitable for use as surrounding mediums if specified. These include, but are not limited to, silicone fluids and other liquids intended for use in transformers, circuit breakers, capacitors, or cables. 
6.4.1.1 The quality of the insulating oil has the potential to have an appreciable effect upon the test results. In addition to the dielectric breakdown voltage, mentioned above, particulate contaminants are especially important when very thin specimens (25 μm (1 mil) or less) are being tested. Depending upon the nature of the oil and the properties of the material being tested, other properties, including dissolved gas content, water content, and dissipation factor of the oil also have the potential to affect the results. Frequent 
replacement of the oil, or the use of filters and other reconditioning equipment is important to minimize the effect of variations of the quality of the oil on the test results. 
6.4.1.2 Breakdown values obtained using liquids having different electrical properties are often not comparable. (SeeX1.4.7.) If tests are to be made at other than room temperature, the bath must be provided with a means for heating or cooling the liquid, and with a means to ensure uniform temperature. Small baths can in some cases be placed in an oven (see 6.4.2) in order to 

 

 


provide temperature control. If forced circulation of the fluid is provided, care must be taken to prevent bubbles from being whipped into the fluid. The temperature shall be maintained within 65°C of the specified test temperature at the electrodes, unless otherwise specified. In many cases it is specified that specimens to be tested in insulating oil are to be previously impregnated with the oil and not removed from the oil before testing (see Practice D2413). For such materials, the bath must be of such design that it will not be necessary to expose the specimens to air before testing. 
6.4.2 If tests in air are to be made at other than ambient temperature or humidity, an oven or controlled humidity chamber must be provided for the tests. Ovens meeting the requirements of Specification D5423 and provided with means for introducing the test voltage will be suitable for use when only temperature is to be controlled. 
6.4.3 Tests in gasses other than air will generally require the use of chambers that can be evacuated and filled with the test gas, usually under some controlled pressure. The design of 
D149 – 094 such chambers will be determined by the nature of the test program to be undertaken 
ASTMD149美標(biāo)標(biāo)準(zhǔn)固體絕緣材料電壓擊穿的實(shí)驗(yàn)方法(十) 
6.5 Test Chamber—The test chamber or area in which the tests are to be made shall be of sufficient size to hold the test equipment, and shall be provided with interlocks to prevent accidental contact with any electrically energized parts. A number of different physical arrangements of voltage source, measuring equipment, baths or ovens, and electrodes are possible, but it is essential that (1) all gates or doors providing access to spaces in which there are electrically energized parts be interlocked to shut off the voltage source when opened; ( 2)clearances are sufficiently large that the field in the area of the electrodes and specimen are not distorted and that flashovers and partial discharges (corona) do not occur except between the test electrodes; and (3) insertion and replacement of specimens between tests be as simple 

 

 


and convenient as possible. Visual observation of the electrodes and test specimen during the test is frequently desirable. 7. Hazards 
7.1 Warning—It is possible that lethal voltages will be present during this test. It is essential that the test apparatus, and all associated equipment electrically connected to it, be properly designed and installed for safe operation. Solidly ground all electrically conductive parts that any person might come into contact with during the test. Provide means for use at the completion of any test to ground any parts which fall into any of the following cases: (a) were at high voltage during the test; (b) have the potential to acquire an induced charge during the test; or (c) have the potential to retain a charge even after disconnection of the voltage source. Thoroughly instruct all operators in the proper way to conduct tests safely. When making high-voltage 
tests,particularly in compressed gas or in oil, it is possible that the energy released at breakdown will be sufficient to result in fire, explosion, or rupture of the test chamber. Design test equipment, test chambers, and test specimens so as to minimize the possibility of such occurrences and to eliminate the possibility of personal injury. 
7.2 Warning—Ozone is a physiologically hazardous gas at elevated 
concentrations. The exposure limits are set by governmental agencies and are usually based upon recommendations made by the American Conference of Governmental ndustrial Hygienists.8 Ozone is likely to be present whenever voltages exist which are sufficient to cause partial, or complete, discharges in air or other atmospheres that contain oxygen. Ozone has a distinctive odor which is initially discernible at low concentrations but sustained inhalation of ozone can cause temporary loss of sensitivity to the scent of ozone. Because of this it is important to measure the concentration of ozone in the atmosphere, using commercially available monitoring devices, whenever the odor of ozone is persistently present or when ozone generating conditions continue. Use appropriate means, such as exhaust vents, to reduce ozone concentrations to acceptable levels in working areas. 8. Sampling 

 

 


8.1 The detailed sampling procedure for the material being tested needs to be defined in the specification for that material. 
8.2 Sampling procedures for quality control purposes shall provide for gathering of sufficient samples to estimate both the average quality and the variability of the lot being examined; and for proper protection of the samples from the time they are taken until the preparation of the test specimens in the laboratory or other test area is begun. 
8.3 For the purposes of most tests it is desirable to take samples from areas that are not immediay adjacent to obvious defects or discontinuities in the material. Avoid the outer few layers of roll material, the top sheets of a package of sheets, or material immediay next to an edge of a sheet or 
roll, unless the presence or proximity of defects or discontinuities is of interest in the investigation of the material. 
8.4 The sample shall be large enough to permit making as many individual tests as required for the particular material (see 12.4). 
9. Test Specimens 
9.1 Preparation and Handling: 
9.1.1 Prepare specimens from samples collected in accordance with Section 8. 9.1.2 When flat-faced electrodes are to be used, the surfaces of the specimens which will be in contact with the electrodes shall be smooth parallel planes, insofar as possible without actual surface machining. 
9.1.3 The specimens shall be of sufficient size to prevent flashover under the conditions of test. For thin materials it will often be convenient to use specimens large enough to permit making more than one test on a single piece. 
9.1.4 For thicker materials (usually more than 2 mm thick) it is possible that the breakdown strength will be high enough that flashover or intense surface partial discharges (corona) will occur prior to breakdown. Techniques that are suitable for use to prevent flashover, or to reduce partial discharge (corona) include: 

 

 


9.1.4.1 Immerse the specimen in insulating oil during the test. See X1.4.7 for the surrounding medium factors influencing breakdown. This is often 
necessary for specimens that have not been dried and impregnated with oil, as well as for those which have been prepared in accordance with Practice D2413,for example. (See 6.4.) 
9.1.4.2 Machine a recess or drill a flat-bottom hole in one or both surfaces of the specimen to reduce the test thickness. If dissimilar electrodes are used (such as Type 6 of Table 1) and only one surface is to be machined, the larger of the two electrodes shall be in contact with the machined surface. Care must be taken in machining specimens not to contaminate or mechanically damage them. 
9.1.4.3 Apply seals or shrouds around the electrodes, in contact with the specimen to reduce the tendency to flashover. 
9.1.5 Materials that are not in flat sheet form shall be tested using specimens (and electrodes) appropriate to the material and the geometry of the sample. It is essential that for these materials both the specimen and the electrodes be defined in the specification for the material. 
8 Available from American Conference of Governmental Industrial Hygienists, Inc. (ACGIH), 1330 Kemper Meadow Dr., Cincinnati, OH 45240, http:// www.acgih.org. D149 – 09 5 
9.1.6 Whatever the form of the material, if tests of other than 
surface-to-surface puncture strength are to be made, define the specimens and the electrodes in the specification for the material. 
9.2 In nearly all cases the actual thickness of the test specimen is important. Unless otherwise specified, measure the thickness after the test in the immediate vicinity of the area of breakdown. Measurements shall be made at room temperature (25 6 5°C), using the appropriate procedure of Test Methods.

主營產(chǎn)品:電壓擊穿試驗(yàn)儀,介電常數(shù)介質(zhì)損耗測(cè)試儀,體積表面電阻率測(cè)試儀,海綿泡沫落球回彈試驗(yàn)儀,介電常數(shù)測(cè)試儀,體積電阻率測(cè)試儀,海綿泡沫壓陷硬度試驗(yàn)儀,介電擊穿強(qiáng)度試驗(yàn)儀,橡膠塑料滑動(dòng)摩擦磨損試驗(yàn)機(jī),耐電弧試驗(yàn)儀,毛細(xì)管流變儀,自動(dòng)進(jìn)樣器,電氣強(qiáng)度試驗(yàn)機(jī),歡迎來電咨詢。
版權(quán)所有©2025 北京北廣精儀儀器設(shè)備有限公司

化工儀器網(wǎng)

推薦收藏該企業(yè)網(wǎng)站
无码高潮少妇毛多水多水免费| 国产VIVODESHD精品| 精品人妻无码区二区三区| 日本多人强伦姧人妻完整版| 亚洲熟妇AV一区二区三区宅男| 吃瓜曝光黑料155FUN| 久久棈精品久久久久久噜噜| 我偷偷跟亲妺作爱H| 48熟女嗷嗷叫国产毛片小说| 国内精品久久久久久久COENT | 被按摩的人妻中文字幕| 精品人妻中文AV一区二区三区 | 中文在线っと好きだっ最新版| 国产精品民宅偷窥盗摄| 欧美专区日韩视频人妻| 亚洲日本中文字幕乱码在线| 被部长灌醉后强行侵犯| 久久人人爽人人爽人人片AV超碰| 十八禁无码免费网站| 最新亚洲人成无码网WWW电影| 国自产拍亚洲免费视频| 三个人一起玩3Q详细经过| 中国成熟妇女毛茸茸| 国产亚洲精品自在久久蜜TV| 日韩少妇白浆无码系列| 又湿又紧又大又爽A视频国产| 国产在线精品无码AV不卡顿| 人妻内射.PORN| 中文字幕人成无码人妻综合社区| 狠狠做五月深爱婷婷| 私人小影院久久久影院| 亚洲日产韩国一二三四区 | 人人妻人人澡人人爽人人老司机| 亚洲6080YY久久无码产自国| JLZZZJLZZZ国产免费观| 老司机精品成人无码AV| 中文在线っと好きだった最新版| 免费无码又爽又高潮视频| A级毛片无码兔费真人久久| 男JI大巴进入女人的视频| 中文字幕亚洲综合久久2020| 国产香蕉97碰碰视频VA碰碰看 | 亚洲中文字幕无码永久在线| 成人精品一区二区三区| 久久久久久亚洲AV无码蜜芽| 亚洲AV成人影视在线观看| 被黑人伦流澡到高潮HNP动漫| 精品国际久久久久999波多野 | 中文字幕无码视频手机免费看| 精品人无码一区二区三区| 无人区码卡二卡WWW| となりの家のネツト在线| 久久亚洲AV成人无码| 亚洲综合久久一区二区| 国产亚洲无日韩乱码| 无码成人一区二区| 低调看JRS直播| 人C交ZZZ0OOZZZ000| 中文字幕无码日韩AV| 久久久久人妻精品一区二区三区| 亚州日本乱码一区二区三区| 国产精品久久久久精品| 少妇下蹲露大唇无遮挡| 出轨 无码 论坛| 日本WINDOWS免费吗| JAPANESE国产永久| 人妻 中文 无码 JAVHD| PYTHON人马大战| 男人一生最吉利的网名| 18禁强伦姧人妻又大又| 看黄A大片爽爽爽不打码| 一区二区国产高清视频在线| 精品免费久久久久久久| 亚洲人成色777777精品百度| 国产三级精品三级男人的天堂 | 午夜影视啪啪免费体验区入口| 国产人妻麻豆蜜桃色精品电影| 亚洲AⅤ天堂AV天堂无码麻豆| 韩国AV一区二区| 亚洲欧洲国无码成人片| 狼人青草久久网伊人| 337P人体粉嫩胞高清大图AV| 琪琪电影网WWW888DVDC| 堕落女教师动漫全无修| 无码人妻丰满熟妇一区二区三区| 国产蜜芽尤物在线一区| 亚洲国产成人精品无码区2021| 久久国产情侣露脸精品| 余生请多指教在线观看免费全集| 女邻居给我口爆18P| 波多野结衣AV无码| 丝袜美女人体艺术| 国产免费久久精品国产传媒| 亚洲国产成人精品无码区二本 | 国产一区内射最近更新| 亚洲日韩AV一区二区三区四区 | 美女高潮潮喷出白浆视频| GOGO西西自慰人体高清人体模| 日韩精品一区二区三区四区蜜桃 | 精品系列无码一区二区三区| 中文字幕大香视频蕉| 人妻人人添人妻人人爱| 国产肥熟女视频一区二区三区 | 中文无码制服丝袜人妻AV| 全免费A级毛片免费看无码| 国产97在线 | 中文| 亚洲AV无码一区二区二三区我 | 伊人久久大香线蕉亚洲| 漂亮人妻偷人精品视频| 国产成人亚洲综合无码DVD| 亚洲精品自偷自拍无码| 年级老师的滋味4| 高潮时粗俗不堪入耳的话| 亚洲爆乳WWW无码专区| 蜜臀AV无码人妻精品| 初尝禁果稚嫩宫交H| 亚洲AV成人午夜福利在线观看| 局长从后面握住我的奶| 成人欧美一区二区三区视频| 亚洲AV成人片色在线观看蜜臀| 老翁的大肉蟒进进出出| 成熟老太毛茸茸BBWBBW| 亚洲AV无码乱码在线观看四虎| 另类极品VPSWINDOWS| 催眠性指导OVA1一6集| 亚洲国产综合精品 在线 一区| 欧美free叉叉叉叉极品少妇| 国产成人亚洲精品另类动态图| 亚洲无线一二三四区手机| 人人妻人人爽人人澡欧美一区| 国产无遮挡又黄又爽在线视频| 中国自产一战二战三战来源| 思思RE热免费精品视频66| 久久精品国产亚洲AV无码娇色| 差差差很疼无掩盖在线观看| 亚洲AV无码AV在线播放| 妞干网在线视频免费观看| 国产精品久久久久久久影院 | 尤物AV无码色AV无码麻豆| 色一情一乱一伦麻豆| 久久精品国产自在天天线| 成人亚洲色欲色一欲WWW| 亚洲日韩乱码中文无码蜜桃臀| 日本护士OOXⅩXXHD| 精品综合久久久久久97超人| 成人免费无码大片A毛片小说| 亚洲精品无码AV专区最新| 人人爽人人澡人人人妻百度| 精品国产一区二区三区久久影院| JAPANESETUBE日本X| 亚洲AV午夜成人片精品电影| 人鲁交YAZHONGHU| 精品无码人妻夜人多侵犯18| 春色精品久久久久午夜aⅴ| 亚洲中文字幕无码人在线 | 国产日韩精品一区二区三区在线观| 77777欧美毛片777777| 亚洲AV性色精品国产小电影| 国产男男Gay做受×Xx男| 99久久婷婷国产综合精品| 亚洲成熟丰满熟妇高潮XXXXX | 无码人妻一区二区三区免费| 男人添女人下部高潮全视频| 国自产精品手机在线观看视频| 暗交小拗女一区二区| 亚洲综合AV色婷婷国产野外| 婷婷五月六月激情综合色中文字幕 | 久久久久久亚洲AV成人无码国产| 国产成人AV一区二区三区无码| 91夜黄性一交一乱一色一情人| 亚洲成AV人片在线观看无APP| 日韩成人一区二区三区在线观看| 久久婷婷五月综合色和啪| 国产老妇伦国产熟女老妇久 | 少妇人妻综合久久中文字幕| 麻豆乱码国产一区二区三区| 国内少妇高潮嗷嗷叫在线播放| 初尝人妻少妇中文字幕| 2018人人看人人爽| 亚洲日韩国产精品乱-久| 无人区码一码二码三码区别图片| 人妻丰满熟妇AⅤ无码区在线电影| 久久天天婷婷五月俺也去| 国产真实自在自偷| 各种少妇BBW撒尿| WWW.色五月.COM| 综合无码成人AⅤ视频在线观看| 亚洲GV天堂无码男同在线观看 | 久久久久99精品成人片直播| 国产猛进猛出又黄又爽又色| 成熟丰满熟妇偷拍XXXXX| 18禁H漫免费漫画无码网站国产| 亚洲欧洲日韩综合色天使| 性欧美VIDEO高清| 天天影视色香欲综合久久| 人人玩人人添人人澡| 国产无遮挡无码很黄很污很刺激| 抖抈短视频APP下载| YEEZY380蜜桃粉满天| 主人给我戴上奶牛榨乳器调教 |